Table 8.

Results of mechanical tests for SDSS joints.

Exp. no. Specimen Heat input (kJ/mm) Tensile strength (MPa) Impact toughness at −46 °C (J) Hardness (VHN)
1 SDSS- Low PREN 0.95 862 140 319
2 1.05 844 130 312
3 1.15 827 126 298
4 1.25 805 107 288
5 SDSS- High PREN 0.75 896 90 326
6 1.0 880 81 320
7 1.1 855 72 315
8 1.2 835 64 302