Mechanical properties of different zones of fusion welded Mg-alloys.

Mg Alloy Hardness Property (HV) Tensile Strength (MPa) References
Tungsten inert gas (TIG) welding
AZ91D   BM: 160; HAZ: 156; WM: 240 [203]
MB3/AZ31 dissimilar BM: 56.8; HAZ:48.1; FZ:52.0 263 MPa, [130]
AZ31 joints HAZ: 15; FZ:73 BM:240 [204]
LA141 Mg-Li-Al BM: 72; FZ: 66 BM: 127; FZ: 124 [64]
AZ31B joints BM:69; FZ: 61 BM: 275; FZ: 220 [75]
AZ31B BM: 62; FZ: 59 BM: 275; FZ: 201 [127]
AZ61 nil BM:250; FZ:230 [126]
AZ31B BM: 52; FZ: 48 BM: 259; FZ: 224 [111]
AZ31B BM: 65; FZ: 58 BM: 280; FZ: 258 [205]
Laser welding
AZ31B-H24 BM: 73; FZ: 54; HAZ: 51 BM: 282; FZ: 254 [95]
AZ31B Mg alloy Nil FZ: 232 [92]
AZ31B Nil BM: 302.2; FZ: 274.1 [134]
AZ31 and AZ61 BM:62; FZ:72 BM:308; FZ:153 [206]
AZ31 FZ: 67.1 Nil [207]
MgAl3Zn1 (AZ31) Nil FZ:240 [138]
AZ61 Mg alloy BM:58; HAZ:56; FZ:64 BM:285; FZ:236 [96]
AZ31B alloy Nil BM:258; FZ:235 [28]
AZ31B and AZ61A Nil BM: 298; FZ: 273 [89]

Current usage metrics show cumulative count of Article Views (full-text article views including HTML views, PDF and ePub downloads, according to the available data) and Abstracts Views on Vision4Press platform.

Data correspond to usage on the plateform after 2015. The current usage metrics is available 48-96 hours after online publication and is updated daily on week days.

Initial download of the metrics may take a while.