For each parameter group, the number of specimens with pores on the fracture surface is given. There were a total of 12 specimens per group. The standard deviation (SD) of the interfacial strength according to IAM/I is also given for each group.
Nozzle temperature | Cooling time | |||||
---|---|---|---|---|---|---|
3.2 s | 9.2 s | 13.7 s | 18.5 s | 23.4 s | ||
190 °C | Specimens width pores | 0 | 0 | 0 | 0 | 0 |
SD of interfacial strength in MPa | 2.81 | 2.41 | 1.44 | 2.82 | 3.86 | |
210 °C | Specimens width pores | 0 | 4 | 5 | 1 | 3 |
SD of interfacial strength in MPa | 1.78 | 2.50 | 4.52 | 1.78 | 6.56 | |
230 °C | Specimens width pores | 0 | 5 | 6 | 7 | 8 |
SD of interfacial strength in MPa | 1.63 | 4.74 | 4.55 | 6.38 | 6.62 |
Current usage metrics show cumulative count of Article Views (full-text article views including HTML views, PDF and ePub downloads, according to the available data) and Abstracts Views on Vision4Press platform.
Data correspond to usage on the plateform after 2015. The current usage metrics is available 48-96 hours after online publication and is updated daily on week days.
Initial download of the metrics may take a while.